Luminescent glass doped with lanthanide oxides (terbium and europium), obtained by using the melt-quenching technique

Material

Glass

Craft

Glass-making

General Technique

Combining

Specific Technique

melt-quenching

Properties & Qualities

Application

Art Product

Qualities

Polished Transparent Other

Colour

Yellow under UV-light

Sample Information

Date of creation

11/08/2011

Recipe Details

SiO2 + CaCO3 + Na2CO3 and the different lanthanide oxides (0.62% Eu2O3 and 2% Tb4O7) were used as starting materials. Approximately 25 g batches were mixed and melted in platinum crucibles in an electric furnace at 1500 °C for 3 h in air. The melted glasses were quenched at room temperature and further annealed at ca. 550 °C for 1 h. The glass samples were cut and carefully polished.

Credits

Craft Maker

Andreia Ruivo

Library Contributor

VICARTE, NOVA

Photographer

Cristiana Prada